Detrimental impact of trace amount of tetrachlorohexafluorobutane impurity in hydrogen on PEM fuel cell performance
Irina Profatilova, Frédéric Fouda-Onana, Marie Heitzmann, Thomas Bacquart, Abigail Morris, John Warren et al. · 2024 · 20 citationsRead the paper
All 8 authors
Frédérique Haloua, Pierre-André Jacques
The presence of various contaminants in hydrogen for automotive polymer electrolyte membrane fuel cells (PEMFCs) can cause detrimental FC system damage. One of the possible sources of fuel pollution is hydrogen storage and distribution facilities. Previously, various isomers of tetrachlorohexafluorobutane (C4Cl4F6) were detected in hydrogen samples from a number of refueling stations. In general, halogenated compounds might have significant negative impact on PEMFC durability. However, the data on their structure/impact on PEMFC relationship is scarce, which complicates ranking of halocarbons in hydrogen quality standards. In this work, the impact of 0.2 ppm of 1,2,3,4-tetrachloro-1,1,2,3,4,4-hexafluorobutane on electrochemical performance of single FC under steady-state and dynamic test protocol of overall 900 h duration is reported for the first time to the best of our knowledge. Detailed in-situ electrochemical study revealed high irreversible voltage losses in a wide range of current densities, impedance growth and anode active surface area degradation provoked by the contaminant in comparison to the cell performance under neat H2. Ex-situ microscopy investigation confirmed thinning and densification of the active anode layer in presence of C4Cl4F6. Energy dispersive X-ray spectroscopy analysis of the aged membrane electrode assemblies evidenced irreversible character of FC contamination by the halogenated impurity. This work contributes to defining a range of important halogenated hydrogen pollutants and to quantification of their impact on PEMFC performance.
What the full text shows
Shown in the lab- Irreversible degradation rate of fuel cell voltage was significantly higher with the contaminant than with pure hydrogen. — -74 μV/h vs -11 μV/h (0.2 ppm C4Cl4F6 in H2 over 900 h at 0.6 A cm-2)
- Significant voltage drop occurred after dynamic load cycling (FC-DLC) despite subsequent cleaning with pure hydrogen. — 71 mV difference (114 mV drop for contaminated vs 43 mV for pure) (0.6 A cm-2 after 530 h of FC-DLC)
- Severe loss of anode electrochemical surface area (ECSA). — 59% loss (0.2 ppm C4Cl4F6 in H2)
- Voltage drop after steady-state phase 2. — 10 mV vs 0 mV for pure H2 (0.6 A cm-2)
- Presence of chlorine atoms in the MEA confirmed by EDX. (Post-mortem analysis of contaminated cell)
- Setup
- 25 cm2 single cell, Gore MX 735.18 membrane, Pt loading 0.11 mg/cm2 (anode) and 0.34 mg/cm2 (cathode), 0.2 ppm C4Cl4F6 in H2.
- How
- The study used a single PEM fuel cell subjected to steady-state and dynamic load cycling (FC-DLC) for 900 hours. In-situ diagnostics included polarization curves, EIS, and cyclic voltammetry, while ex-situ analysis used FEG-SEM and EDX.
- Limitations
- Technical limitations in preparing precise, stable gas mixtures at very low concentrations. · Limited understanding of the exact chemical transformations of C4Cl4F6 inside the cell.
Summarized by Gemma 4 from the open-access full text · 8 Oct 2026. Read it