Mechanical properties of thermoformed and direct-printed aligner materials after immersion in 37 °C water: a 14-day in vitro study
Rodrigo Oyonarte, Isabel Lagos, F. L., Tomás Parada B., Alberto del Real, SoonHo Jang et al. · 2026 · 3 citationsRead the paper
All 12 authors
Harim Jeong, Jiho Lee, Jinhong Min, Tarek M. Elshazly, Jung-Yul Cha, Hoon Kim
This study compared the mechanical properties of direct-printed dental aligner materials made from 3D-printed resins TC-85, TR-07, and TA-28 with those of two conventional thermoformed materials—Zendura-A and Zendura-Flx—to evaluate their performance under simulated physiological conditions. Test specimens were immersed in a 37 °C water bath for 12 different durations: 0, 5, and 30 min; 1, 3, 6, and 9 h; and 1, 3, 7, and 14 d. Tensile tests were performed using a universal testing machine (Zwick Z010, Zwick, Ulm, Germany) to measure the Young’s modulus (MPa), elongation at break (%), and tensile force (N) at strains of 1%, 2%, and 3%. After 14 d of immersion, TC-85, TA-28, and TR-07 exhibited forces in the range of 4.04–7.24 N at 1% strain and 7.30–13.48 N at 3% strain, while Zendura A and Zendura FLX exhibited forces of 26.26–32.91 N at 1% strain and 32.91–65.23 N at 3% strain. The Young’s modulus and UTS results exhibit a trend similar to that of the tensile force. Direct-printed aligners exhibited a 25.3% (TC-85) increase in elongation at break after 30 min, whereas thermoformed aligners exhibited a 5.5% reduction. Direct-printed resins, such as TC-85, TA-28, and TR-07, with temperature-responsive viscoelastic behavior, exhibited statistically significant differences from thermoformed aligner materials, delivering lower mechanical loads that could favor a more suitable orthodontic force profile for clear aligners.
What the full text shows
Shown in the lab- Direct-printed resins (TC-85, TA-28, TR-07) deliver significantly lower tensile forces at body temperature compared to thermoformed materials. — 4.04–13.48 N vs. 26.26–65.23 N (at 1%–3% strain after 14d) (37 °C water immersion for 14 days)
- Direct-printed resins exhibit a rapid reduction in Young's modulus (stiffness) upon immersion. — TC-85: 1169.8 to 289.58 MPa; TA-28: 1401.6 to 311.1 MPa; TR-07: 1259.4 to 560.18 MPa (0 to 14 days immersion at 37 °C)
- Thermoformed materials maintain significantly higher ultimate tensile strength (UTS) than direct-printed resins. — Zendura A: 58.76–72.44 MPa vs. TC-85: 14.38–24.29 MPa (37 °C water immersion)
- Direct-printed materials show increased elongation at break after immersion, while thermoformed materials remain stable. — TC-85: 75.54% to 111.5% increase (0 to 14 days immersion at 37 °C)
- Thermoforming causes significant material thinning, while 3D printing increases thickness over design values. — Zendura A: 45.5% reduction; Direct-printed: 40–46% increase (Post-manufacturing measurement)
- Setup
- 385 specimens (n=7 per group) across 5 materials (TC-85, TR-07, TA-28, Zendura-A, Zendura-Flx) and 11 immersion time points.
- How
- Tensile testing (Young's modulus, UTS, elongation, and force at 1-3% strain) was performed on dumbbell-shaped specimens of 3D-printed resins and thermoformed sheets after immersion in a 37 °C water bath for durations up to 14 days.
- Limitations
- Uniaxial tensile testing of flat specimens does not replicate complex intraoral loading and geometry. · In vitro study lacks real-world variables like saliva and fluctuating temperature. · Lack of standard testing methods for comparing different fabrication processes.
Summarized by Gemma 4 from the open-access full text · 8 Oct 2026. Read it